Applications:
High strength drawn tubing.
Characteristic Properties:
Heat treatable alloy. High mechanical strength slightly higher than 2011 and 2017A.
|
BS 3L63(1971) Alloy 3L63 |
|
|---|---|
| Chemical Element | % Present |
| Aluminium (Al) | balance |
| Tin (Sn) | 0.05 max |
| Lead (Pb) | 0.05 max |
| Chromium (Cr) | 0.1 max |
| Nickel (Ni) | 0.2 max |
| Zinc (Zn) | 0.2 max |
| Titanium + Zirconium (Ti+Zr) | 0.2 max |
| Iron (Fe) | 0.5 max |
| Magnesium (Mg) | 0.2 - 0.8 |
| Silicon (Si) | 0.5 - 0.9 |
| Manganese (Mn) | 0.4 - 1.2 |
| Copper (Cu) | 3.9 - 5 |
Aluminium alloy 3L63 - 2014A is covered by standard BS EN 4L63 (1971)
The most common tempers for 3L63 - 2014A aluminium tubing is:
3L63 - 2014A aluminium is supplied as drawn tube
| Physical Property | Value |
|---|---|
| Density | 2.8 g/cm³ |
| Melting Point | 640 °C |
| Thermal Expansion | 22.8 x10^-6 /K |
| Modulus of Elasticity | 73 GPa |
| Thermal Conductivity | 134-155 W/m.K |
|
BS 3L63(1971) Tube - |
|
|---|---|
| Mechanical Property | Value |
| Proof Stress | 370 Min MPa |
| Tensile Strength | 450 Min MPa |
| Elongation A50 mm | 7 Min % |